Carbon steel grades: types, numbering and common grades
Carbon steel grades use the SAE/AISI four-digit system: the first two digits give the family (10xx plain carbon, 11xx free-machining, 41xx chromium-molybdenum) and the last two give carbon in hundredths of a percent, so 1045 has about 0.45 % carbon. Low carbon steel has up to about 0.25–0.30 % carbon, medium 0.30–0.60 % and high 0.60–1.0 % or more.

Key takeaways
- In an SAE/AISI number the last two digits are the nominal carbon in hundredths of a percent: 1018 has about 0.18 % C.
- Low carbon (mild) steel has up to about 0.25–0.30 % carbon, medium 0.30–0.60 %, high 0.60–1.0 % and above.
- Higher carbon steel is harder and stronger after heat treatment but less ductile and harder to weld.
- 4140 is a chromium-molybdenum alloy steel that through-hardens in oil; 1045 is plain carbon and hardens only in thin sections or at the surface.
- Equivalents such as 1045, C45, S45C and GB 45 are nearest matches; the standard and mill certificate decide.
What are carbon steel grades?
Carbon steel grades are standardized iron-carbon alloys named by the SAE/AISI four-digit system, such as 1018, 1045 or 1095. The first two digits give the alloy family and the last two digits give the nominal carbon content in hundredths of a percent, so 1045 is a plain carbon steel with about 0.45 % carbon.
Carbon steel is steel whose properties come mainly from its carbon content, with only small amounts of manganese, silicon and copper and no specified minimum of chromium, nickel or molybdenum. Carbon is the element that decides how hard and strong the steel can get. More carbon means more strength and hardenability, and less ductility and weldability.
In practice "carbon steel grades" usually covers two groups that share the same numbering system: plain carbon steels (10xx, 11xx, 12xx, 15xx) and low-alloy steels (41xx, 43xx, 86xx and others). Low-alloy steels such as 4140 add small amounts of chromium, molybdenum or nickel, typically a few percent in total, to harden deeper in thicker sections. Stainless steel, with at least 10.5 % chromium, is a separate family covered in stainless steel grades explained.
Types of carbon steel: low, medium and high carbon
Carbon steel is split into three types by carbon content: low carbon (up to about 0.25–0.30 %), medium carbon (about 0.30–0.60 %) and high carbon (about 0.60–1.0 % and above). The boundaries are conventions, not fixed by one standard, so sources differ by a few hundredths of a percent.
| Type | Carbon, % | Common grades | Hardens by quenching? | Weldability | Typical uses |
|---|---|---|---|---|---|
| Low carbon (mild steel) | up to about 0.25–0.30 | 1008, 1018, 1020, A36, 12L14 | No, only case hardening | Excellent | Sheet, plate, structural shapes, brackets, pins |
| Medium carbon | about 0.30–0.60 | 1035, 1045, 1050, 1144 | Yes, in thin sections or at the surface | Fair, needs preheat | Shafts, axles, gears, forgings |
| High carbon | about 0.60–1.0 and above | 1060, 1075, 1080, 1095 | Yes, to high hardness | Poor | Springs, blades, cutting edges, wire |
Low carbon steel
Low carbon steel is soft, ductile and easy to weld, bend and form. It does not respond usefully to quench hardening because there is too little carbon to form hard martensite. Parts that need a hard surface are carburized or carbonitrided, which adds carbon to the outer layer only.
Medium carbon steel
Medium carbon steel balances strength and toughness. Grades such as 1045 are supplied hot rolled, normalized or cold drawn, and are often flame or induction hardened at the wearing surface. Welding needs preheat and controlled cooling to avoid cracking in the heat-affected zone.
High carbon steel
High carbon steel reaches the highest hardness of the plain carbon steels after quenching and is used for springs and edges. It is brittle if left untempered and is rarely welded. Above about 1 % carbon, plain carbon steels shade into the carbon tool steels (W class), covered in tool steel grades.
Is higher carbon steel harder or softer? Harder. At the same heat treatment, more carbon gives higher hardness and strength. The maximum as-quenched hardness of steel rises steeply with carbon up to roughly 0.6 %, then levels off. See the steel hardness chart for how hardness scales compare.
How the SAE/AISI steel numbering system works
An SAE/AISI steel number has four digits (five for some high-carbon grades such as 52100). The first two digits name the family; the last two give the nominal carbon in hundredths of a percent. A letter L between the digits, as in 12L14, means lead was added for machinability; a B, as in 15B41, means boron was added for hardenability.
| Series | Family | Main additions | Example |
|---|---|---|---|
| 10xx | Plain carbon | Manganese 1.00 % max | 1018, 1045, 1095 |
| 11xx | Resulfurized free-machining | Sulfur for chip breaking | 1117, 1144 |
| 12xx | Resulfurized and rephosphorized free-machining | Sulfur and phosphorus | 1215, 12L14 |
| 15xx | Plain carbon, high manganese | Manganese over 1.00 % | 1524, 1541 |
| 41xx | Chromium-molybdenum | Cr and Mo | 4130, 4140 |
| 43xx | Nickel-chromium-molybdenum | Ni about 1.8 %, Cr, Mo | 4340 |
| 51xx | Chromium | Cr | 5160 |
| 52xxx | High-carbon chromium (bearing) | Cr, about 1 % C | 52100 |
| 86xx | Nickel-chromium-molybdenum | Small Ni, Cr, Mo | 8620 |
Reading an example: 4140 is a 41xx chromium-molybdenum steel with 0.40 % nominal carbon (0.38–0.43 % actual range). 1018 is a 10xx plain carbon steel with 0.18 % nominal carbon (0.15–0.20 %). The number does not tell you the condition, such as hot rolled, cold drawn, annealed or quenched and tempered. That is stated separately on the order and the mill certificate.
Structural steels are an exception. A36 and A572 Grade 50 are ASTM specification names, not SAE numbers, and they are specified mainly by minimum strength rather than by exact chemistry.
Common carbon steel grades chart
The grades below cover most carbon and low-alloy bar, plate and tube bought by machine shops. Carbon ranges are per SAE J403 and ASTM A29 for bar; A36 carbon limits per ASTM A36 depend on product form and thickness. Machinability ratings are qualitative and depend on condition.
| Grade | Type | Carbon, % | Typical uses | Machinability |
|---|---|---|---|---|
| 1018 | Low carbon (mild) | 0.15–0.20 | Pins, shafts, spacers, bushings, fixtures, carburized parts | Good, best cold drawn |
| 1020 | Low carbon (mild) | 0.18–0.23 | Brackets, light shafts, welded fabrications, carburized parts | Good, can be gummy |
| A36 | Low carbon structural | 0.25–0.29 max | Plate, beams, base plates, frames, general fabrication | Fair, abrasive mill scale |
| 12L14 | Low carbon, resulfurized, rephosphorized and leaded | 0.15 max | High-volume screw-machine parts, fittings, inserts | Excellent, poor weldability |
| 1045 | Medium carbon | 0.43–0.50 | Shafts, axles, gears, studs, couplings, induction-hardened parts | Good |
| 1144 | Medium carbon, resulfurized | 0.40–0.48 | Shafts and spindles machined in volume, hydraulic rods | Very good, poor weldability |
| 1095 | High carbon | 0.90–1.03 | Springs, blades, cutting edges, wear parts | Fair annealed |
| 4130 | Cr-Mo alloy (chromoly) | 0.28–0.33 | Tube frames, roll cages, aircraft and motorsport parts | Good normalized |
| 4140 | Cr-Mo alloy | 0.38–0.43 | Shafts, spindles, gears, tool holders, high-strength studs | Good annealed, fair pre-hardened |
| 4340 | Ni-Cr-Mo alloy | 0.38–0.43 | Heavy shafts, crankshafts, landing gear, highly loaded parts | Fair |
| 8620 | Ni-Cr-Mo alloy, case hardening | 0.18–0.23 | Carburized gears, pinions, camshafts | Good |
What is 1018 steel? 1018 is a low-carbon plain carbon steel with 0.15–0.20 % carbon and 0.60–0.90 % manganese, usually sold as cold-drawn bar. It machines and welds well, takes a good finish and is a common choice for pins, spacers and fixture parts. It is case hardened by carburizing when a hard surface is needed. Typical strength figures are in the steel properties chart.
12L14 and 1144 are free-machining grades. Sulfur forms manganese sulfide inclusions that break chips; lead in 12L14 lubricates the cut. Both trade weldability and some toughness for speed. Use them for turned parts that will not be welded.
Mild steel grades and carbon steel vs mild steel
Mild steel is low carbon steel, usually with about 0.05–0.25 % carbon. All mild steel is carbon steel, but not all carbon steel is mild steel: 1045 and 1095 are carbon steels that are not mild. Common mild steel grades are 1008, 1010, 1018, 1020, A36 and, in Europe, S235 and S275.
Mild steel is chosen when welding, bending and low cost matter more than strength or hardness. A36 has a minimum yield strength of 250 MPa (36 ksi) and a tensile strength of 400–550 MPa (58–80 ksi) under ASTM A36. Like all carbon steel, mild steel has a density of about 7.85 g/cm³ (0.284 lb/in³) and rusts if left unprotected.
Is stainless steel stronger than mild steel? Not by default. Annealed 304 stainless has a minimum yield strength of 205 MPa (30 ksi), below A36, but a higher minimum tensile strength of 515 MPa (75 ksi) and it work-hardens quickly. Hardened martensitic and duplex stainless grades are much stronger than mild steel.
Alloy steel vs carbon steel
Alloy steel adds deliberate amounts of chromium, molybdenum, nickel, vanadium or other elements to carbon steel. The main gain is hardenability: an alloy steel hardens through a thicker section with a less severe quench, which means less distortion and cracking.
| Property | Plain carbon steel (10xx) | Low-alloy steel (41xx, 43xx, 86xx) |
|---|---|---|
| Alloying | Carbon and manganese only | Adds Cr, Mo, Ni, V in small amounts |
| Hardenability | Shallow; water or brine quench for full hardness | Deeper; oil quench is usual |
| Toughness after hardening | Lower | Higher at the same hardness |
| Cost | Lowest | Higher |
| Weldability | Excellent for low carbon | Needs preheat; 4130 is the most weldable common grade |
1045 vs 4140 steel
1045 is a plain medium-carbon steel; 4140 is a chromium-molybdenum alloy steel with about the same carbon. Choose 1045 for lower cost and surface hardening; choose 4140 when the part must be hard and tough through its section.
| Point | 1045 | 4140 |
|---|---|---|
| Carbon, % | 0.43–0.50 | 0.38–0.43 |
| Alloying | None beyond manganese | Cr 0.80–1.10 %, Mo 0.15–0.25 % |
| Through-hardening | Thin sections only | Moderate sections, oil quench |
| Usual supply condition | Hot rolled, normalized or cold drawn | Annealed or pre-hardened (typically 28–32 HRC) |
| Common hardening route | Induction or flame hardening of the surface | Quench and temper, or buy pre-hardened |
| Typical parts | Shafts, axles, pins, gears | Highly loaded shafts, spindles, tool holders, studs |
4140 costs more per pound but saves a heat-treatment step when bought pre-hardened. For quench-and-temper details see heat treating 4140 steel. 4340 adds about 1.65–2.00 % nickel to the same base and hardens deeper still, for heavy sections that must stay tough.
Carbon steel equivalents: AISI, EN, JIS and GB
Each AISI grade has a nearest equivalent in European (EN), Japanese (JIS) and Chinese (GB) standards. They are nearest matches, not identical grades: composition limits and required properties differ in detail.
| AISI / ASTM | EN name | EN number | JIS | China GB | Type |
|---|---|---|---|---|---|
| 1020 | C22 | 1.0402 | S20C | 20 | Low-carbon steel |
| 1045 | C45 | 1.0503 | S45C | 45 | Medium-carbon steel |
| 4130 | 25CrMo4 | 1.7218 | SCM430 | 30CrMo | Chromium-molybdenum alloy steel |
| 4140 | 42CrMo4 | 1.7225 | SCM440 | 42CrMo | Chromium-molybdenum alloy steel |
| 8620 | 20NiCrMo2-2 | 1.6523 | SNCM220 | 20CrNiMo | Nickel-chromium-molybdenum case-hardening steel |
| 52100 | 100Cr6 | 1.3505 | SUJ2 | GCr15 | High-carbon chromium bearing steel |
| A36 | S235JR | 1.0038 | SS400 | Q235B | Structural carbon steel |
| A572 Gr 50 | S355JR | 1.0045 | SM490A | Q355B | High-strength low-alloy structural steel |
Structural grades need the most care. A36, S235JR, SS400 and Q235B specify different minimum strengths and test requirements, so do not swap them on a structural drawing without an engineer's check. The full list is on the steel grade equivalents page. When machining these grades, start with the tap drill chart and drill bits for metal; medium-carbon and alloy steels are also the base of SAE Grade 5 and Grade 8 bolts.
Sources and standards
- SAE J403
- ASTM A29
- ASTM A36
- ASTM A240
- EN 10083
- EN 10025-2
- JIS G 4051
- JIS G 4053
General reference information. When a manufacturer, drawing or governing standard gives a value, that value takes precedence.
Related charts and guides
Common questions
Is higher carbon steel harder or softer?
Higher carbon steel is harder. With the same heat treatment, more carbon gives higher hardness and strength but lower ductility and weldability. Maximum as-quenched hardness rises steeply with carbon up to about 0.6 % and then levels off, which is why springs and blades use 0.60–1.0 % carbon steel.
What is 1018 steel?
1018 is a low-carbon plain carbon steel with 0.15–0.20 % carbon and 0.60–0.90 % manganese, usually supplied as cold-drawn bar. It machines and welds well and is used for pins, spacers, shafts and fixture parts. It cannot be through-hardened but can be carburized for a hard surface.
What is the difference between carbon steel and mild steel?
Mild steel is a type of carbon steel: low carbon steel with about 0.05–0.25 % carbon, such as 1018, 1020 or A36. Carbon steel also includes medium and high carbon grades such as 1045 and 1095, which are stronger and hardenable but harder to weld. All mild steel is carbon steel, not the reverse.
What do the numbers in 1045 or 4140 mean?
In the SAE/AISI system the first two digits name the steel family and the last two give the nominal carbon in hundredths of a percent. 1045 is a 10xx plain carbon steel with about 0.45 % carbon. 4140 is a 41xx chromium-molybdenum steel with about 0.40 % carbon, actual range 0.38–0.43 %.
What is the difference between alloy steel and carbon steel?
Carbon steel relies on carbon and manganese only. Alloy steel adds small amounts of chromium, molybdenum, nickel or vanadium, which let it harden through thicker sections with a milder oil quench and give better toughness at the same hardness. Low-alloy steels such as 4140 and 4340 use the same SAE/AISI numbering as carbon steels.
Is stainless steel stronger than mild steel?
Not always. Annealed 304 stainless has a minimum yield strength of 205 MPa (30 ksi), lower than the 250 MPa (36 ksi) of A36 mild steel, but a higher minimum tensile strength of 515 MPa (75 ksi). Stainless work-hardens quickly, and hardened martensitic or duplex stainless grades are much stronger than mild steel.
What is a medium carbon steel?
Medium carbon steel has about 0.30–0.60 % carbon. Common grades are 1035, 1045, 1050 and the free-machining 1144. It is stronger than mild steel and can be hardened in thin sections or at the surface by induction or flame hardening. It is used for shafts, axles, gears and forgings and needs preheat for welding.