Short answer

Typical steel properties: carbon steel density 7.85 g/cm³ (0.284 lb/in³), Young's modulus 200–210 GPa (29–30 Msi), thermal expansion 11–13 µm/m·°C, conductivity 45–55 W/m·K and melting range about 1425–1540 °C. 304 stainless is about 7.93 g/cm³, 193 GPa, 17.3 µm/m·°C and 16 W/m·K, and melts at about 1400–1450 °C.

By the MachinistCharts editors · Updated · 7 min read · Checked against EN 10088-1

Carbon steel plate, stainless round bar and square bar beside a caliper and scale

Key takeaways

  • Carbon steel density is 7.85 g/cm³ (0.284 lb/in³); 304 is about 7.93 and 316 about 8.0 g/cm³.
  • Young's modulus is about 200–210 GPa (29–30 Msi) for carbon steel and about 193 GPa (28 Msi) for 304 and 316.
  • Heat treatment changes strength, not stiffness: modulus is nearly the same for annealed and hardened steel.
  • 304 and 316 annealed have a minimum yield strength of 205 MPa (30 ksi) and tensile strength of 515 MPa (75 ksi) per ASTM A240.
  • Steel weight = volume × density; round bar in kg/m = 0.006165 × d² with d in mm.

Steel properties chart: physical properties of steel

Carbon steel has a density of about 7.85 g/cm³ (0.284 lb/in³), a Young's modulus of about 200–210 GPa (29–30 Msi) and melts at about 1425–1540 °C (2600–2800 °F). Austenitic stainless steels such as 304 and 316 are slightly denser, slightly less stiff, expand more with heat and conduct heat about a third as well.

Physical properties such as density, modulus and thermal expansion change little between grades in one family, so one typical value serves for most design work. Strength and hardness, by contrast, depend strongly on grade and condition and are covered further down. All values below are typical, near room temperature unless stated.

PropertyCarbon and low-alloy steel304 stainless316 stainless
Density7.85 g/cm³ (0.284 lb/in³)7.93–8.00 g/cm³ (0.286–0.289 lb/in³)about 8.0 g/cm³ (0.289 lb/in³)
Young's modulus (E)200–210 GPa (29–30 Msi)about 193 GPa (28 Msi)about 193 GPa (28 Msi)
Shear modulus (G)about 79–80 GPa (11.5 Msi)lower than carbon steel; see maker's data
Poisson's ratio0.29–0.30about 0.27–0.30about 0.27–0.30
Thermal expansion, 20–100 °C11–13 µm/m·°C (6.1–7.2 µin/in·°F)about 17.3 µm/m·°C (9.6 µin/in·°F)about 16.0 µm/m·°C (8.9 µin/in·°F)
Thermal conductivityabout 45–55 W/m·K (26–32 BTU/h·ft·°F); about 42 for 4140about 16 W/m·K (9.2 BTU/h·ft·°F)about 16 W/m·K (9.2 BTU/h·ft·°F)
Specific heat0.46–0.49 J/g·K (0.11–0.12 BTU/lb·°F)about 0.50 J/g·K (0.12 BTU/lb·°F)about 0.50 J/g·K (0.12 BTU/lb·°F)
Melting rangeabout 1425–1540 °C (2600–2800 °F)about 1400–1450 °C (2550–2650 °F)about 1375–1400 °C (2500–2550 °F)
Electrical resistivity, 20 °Cabout 0.15–0.20 µΩ·mabout 0.72 µΩ·mabout 0.74 µΩ·m
MagneticYesNo when annealedNo when annealed

For other stainless grades and how they differ, see stainless steel grades explained and 304 vs 316 stainless steel.

Steel density and stainless steel density

The standard density of carbon steel is 7.85 g/cm³, which is 7850 kg/m³, 0.284 lb/in³ or 490 lb/ft³. Stainless steel density is 7.7–8.0 g/cm³ depending on grade: ferritic grades are lightest, austenitic 304 and 316 heaviest.

MaterialDensityNote
Carbon and low-alloy steel (1018, 1045, 4140, A36)7.85 g/cm³ (0.284 lb/in³, 490 lb/ft³)Standard design value
304 / 304L stainless7.93 g/cm³ (0.286 lb/in³, 495 lb/ft³)Some data sheets give 8.00
316 / 316L stainless8.00 g/cm³ (0.289 lb/in³, 499 lb/ft³)Typical
430 ferritic stainless7.70 g/cm³ (0.278 lb/in³, 481 lb/ft³)Typical; about 7.7–7.75
Pure iron7.874 g/cm³ (0.284 lb/in³, 492 lb/ft³)Reference value

The difference matters for weight estimates: 316 bar weighs about 2 % more than the same carbon steel bar. Alloying elements change density only slightly, so 1018, 1045, 4140 and A36 all use 7.85 g/cm³.

Modulus of elasticity of steel

The modulus of elasticity of steel, also called Young's modulus or tensile modulus, is about 200–210 GPa (29–30 Msi) for carbon and alloy steel and about 193 GPa (28 Msi) for 304 and 316 stainless. Common design values are 200 GPa in metric work and 29,000 ksi in US structural work.

Modulus sets stiffness: how far a part deflects under a load below its yield point. It barely changes with grade or heat treatment. A hardened 4140 shaft deflects the same as an annealed 1018 shaft of the same size under the same load; heat treatment only raises the load at which it yields. To make a part stiffer, change its shape, not its grade.

The shear modulus (G) of carbon steel is about 79–80 GPa (11.5 Msi) and Poisson's ratio is about 0.29–0.30. They are linked by G = E / (2 × (1 + ν)): with E = 205 GPa and ν = 0.29, G ≈ 79 GPa.

Thermal properties of steel: expansion, conductivity, specific heat and melting point

Thermal expansion coefficient of steel

Carbon steel expands about 11–13 µm per meter per °C (6.1–7.2 µin/in·°F); a common single value is 12 µm/m·°C. Austenitic stainless expands about 16–17.3 µm/m·°C, about 40 % more. A 1 m carbon steel bar heated by 50 °C grows about 0.6 mm; a 304 bar grows about 0.85 mm. This is why stainless fixtures move more during welding and why shrink fits depend on the expansion coefficient.

Thermal conductivity of stainless steel and carbon steel

Carbon steel conducts heat at about 45–55 W/m·K, falling to about 42 W/m·K in alloy steel such as 4140. 304 and 316 stainless conduct only about 15–16 W/m·K. Heat stays at the cutting zone in stainless, which is one reason it work-hardens and wears tools faster.

Specific heat of steel and iron

The specific heat of pure iron is about 0.449 J/g·K (0.107 BTU/lb·°F) at room temperature. Carbon steel is about 0.46–0.49 J/g·K and stainless about 0.50 J/g·K. Specific heat rises with temperature, so heat-treatment energy calculations at furnace temperature need higher values.

Stainless steel melting point

Steel melts over a range, not at one temperature. Carbon steel melts at about 1425–1540 °C (2600–2800 °F), with higher carbon lowering the range; pure iron melts at 1538 °C (2800 °F). 304 stainless melts at about 1400–1450 °C (2550–2650 °F) and 316 at about 1375–1400 °C (2500–2550 °F). Useful strength is lost far below melting, so service temperature limits are set by strength and oxidation, not by melting point.

Yield strength and tensile strength of steel

Yield strength is the stress at which steel starts to deform permanently, usually measured at 0.2 % offset. Tensile strength (ultimate tensile strength) is the highest stress the steel reaches before it necks and breaks. Both depend on grade and condition, so the standard sets minimums and the mill certificate reports the actual values.

Grade and conditionYield strengthTensile strengthBasis
A36 structural steel250 MPa (36 ksi) min400–550 MPa (58–80 ksi)ASTM A36
A572 Grade 50345 MPa (50 ksi) min450 MPa (65 ksi) minASTM A572
S235JR, up to 16 mm thick235 MPa min360–510 MPaEN 10025-2
S355JR, up to 16 mm thick355 MPa min470–630 MPaEN 10025-2
1018, cold drawnabout 370 MPa (54 ksi)about 440 MPa (64 ksi)Typical
1045, cold drawnabout 530 MPa (77 ksi)about 625 MPa (91 ksi)Typical
4140, annealedabout 415 MPa (60 ksi)about 655 MPa (95 ksi)Typical
304 and 316, annealed205 MPa (30 ksi) min515 MPa (75 ksi) minASTM A240
304L and 316L, annealed170 MPa (25 ksi) min485 MPa (70 ksi) minASTM A240
2205 duplex (S32205)450 MPa (65 ksi) min655 MPa (95 ksi) minASTM A240

What is the maximum yield strength of steel? There is no single figure. Mild steel yields at about 250 MPa, quenched and tempered alloy steels reach well over 1,000 MPa, and some maraging and specialty steels exceed 2,000 MPa. Strength rises with hardness: the steel hardness chart gives an approximate tensile strength for each HRC value. For bolt strengths, see bolt grades and markings.

Steel weight formula for plate and bar

Steel weight = volume × density. Use 7.85 g/cm³ (7850 kg/m³, 0.2836 lb/in³) for carbon steel and about 7.93–8.0 g/cm³ for 304 and 316 stainless.

  • Plate, metric: weight (kg) = length (m) × width (m) × thickness (mm) × 7.85
  • Plate, inch: weight (lb) = length (in) × width (in) × thickness (in) × 0.2836
  • Round bar, metric: kg/m = 0.006165 × d² (d in mm)
  • Round bar, inch: lb/ft = 2.673 × d² (d in in)
  • Square bar, metric: kg/m = 0.00785 × a² (a = side in mm)

Worked examples

Plate, metric: 1000 × 500 × 10 mm carbon steel. Volume = 1.0 m × 0.5 m × 0.010 m = 0.005 m³. Weight = 0.005 × 7850 = 39.25 kg.

Plate, inch: 12 × 12 × 1/2 in carbon steel. Volume = 72 in³. Weight = 72 × 0.2836 = 20.4 lb.

Round bar: 50 mm diameter, 2 m long. Weight = 0.006165 × 50² × 2 = 30.8 kg. The same bar in 316 stainless weighs about 2 % more.

Steel bar weight chart

Calculated from 7.85 g/cm³. Multiply by 1.01 for 304 or 1.02 for 316 stainless.

Size (diameter or side)Round bar, kg/mSquare bar, kg/m
10 mm0.620.79
12 mm0.891.13
16 mm1.582.01
20 mm2.473.14
25 mm3.854.91
30 mm5.557.07
40 mm9.8612.56
50 mm15.4119.62
60 mm22.2028.26
80 mm39.4650.24
100 mm61.6578.50
Size (diameter or side)Round bar, lb/ftSquare bar, lb/ft
1/2 in0.670.85
3/4 in1.501.91
1 in2.673.40
1-1/4 in4.185.32
1-1/2 in6.017.66
2 in10.6913.61
2-1/2 in16.7121.27
3 in24.0630.63
4 in42.7754.45

For converting fractional sizes, use the inch to mm chart. Grade names and international equivalents are on the steel grade equivalents page, and grade families are explained in carbon steel grades and tool steel grades.

Sources and standards

  • EN 10088-1, Stainless steels, list of stainless steels
  • ASTM A36
  • ASTM A572
  • ASTM A240
  • EN 10025-2

General reference information. When a manufacturer, drawing or governing standard gives a value, that value takes precedence.

Related charts and guides

Common questions

What is the density of stainless steel?

Stainless steel density is about 7.7–8.0 g/cm³ depending on grade. 304 is about 7.93 g/cm³ (0.286 lb/in³) and 316 about 8.0 g/cm³ (0.289 lb/in³). Ferritic 430 is lighter at about 7.7 g/cm³. Carbon steel, for comparison, is 7.85 g/cm³ (0.284 lb/in³).

What is the melting point of stainless steel?

Stainless steel melts over a range rather than at one temperature. 304 melts at about 1400–1450 °C (2550–2650 °F) and 316 at about 1375–1400 °C (2500–2550 °F). Carbon steel melts at about 1425–1540 °C (2600–2800 °F), and pure iron at 1538 °C (2800 °F).

What is the modulus of elasticity of steel?

The modulus of elasticity (Young's modulus) of carbon and alloy steel is about 200–210 GPa, or 29–30 million psi. 304 and 316 stainless are about 193 GPa (28 million psi). Common design values are 200 GPa and 29,000 ksi. Modulus hardly changes with heat treatment, so hardened and annealed steel are equally stiff.

What is the yield strength of 304 stainless steel?

Annealed 304 stainless steel has a minimum yield strength of 205 MPa (30 ksi) and a minimum tensile strength of 515 MPa (75 ksi) under ASTM A240. 304L is lower at 170 MPa (25 ksi) yield and 485 MPa (70 ksi) tensile. Cold-worked 304 is much stronger; the mill certificate gives actual values.

What is the thermal expansion coefficient of steel?

Carbon steel expands about 11–13 µm/m·°C (6.1–7.2 µin/in·°F) between 20 and 100 °C; 12 µm/m·°C is a common single value. Austenitic stainless such as 304 expands about 17.3 µm/m·°C and 316 about 16.0 µm/m·°C. A 1 m carbon steel bar heated by 50 °C grows about 0.6 mm.

What is the specific heat of iron and steel?

Pure iron has a specific heat of about 0.449 J/g·K (0.107 BTU/lb·°F) at room temperature. Carbon steel is about 0.46–0.49 J/g·K and 304 and 316 stainless about 0.50 J/g·K. Specific heat rises with temperature, so use higher values for calculations at heat-treatment temperatures.

What is the thermal conductivity of stainless steel?

304 and 316 stainless steel conduct heat at about 16 W/m·K (about 9.2 BTU/h·ft·°F) near room temperature. That is about one third of carbon steel at 45–55 W/m·K. The low conductivity keeps heat at the cutting edge when machining stainless and makes stainless parts distort more when welded.

How do you calculate the weight of steel?

Multiply volume by density. For carbon steel plate, weight in kg = length (m) × width (m) × thickness (mm) × 7.85; in pounds, multiply cubic inches by 0.2836. Round bar weighs 0.006165 × d² kg/m with d in mm, or 2.673 × d² lb/ft with d in inches. Stainless is 1–2 % heavier.