304 vs 316 stainless steel: differences, strength and uses

Short answer

The difference between 304 and 316 stainless steel is 2–3 % molybdenum in 316, plus more nickel. Molybdenum raises the typical PREN from about 18–20 for 304 to 24–26 for 316, so 316 resists salt and chlorides far better. Both have the same ASTM A240 annealed minimums: 515 MPa (75 ksi) tensile, 205 MPa (30 ksi) yield. 316 typically costs 20–40 % more.

By the MachinistCharts editors · Updated · 7 min read · Checked against EN 10088-1

Two matching stainless steel bars and pipe pieces side by side with bolts on a surface plate

Key takeaways

  • 316 adds 2–3 % molybdenum and 10–14 % nickel; 304 is about 18 % chromium and 8 % nickel.
  • Typical PREN is about 18–20 for 304 and 24–26 for 316, so 316 resists chlorides better.
  • Annealed 304 and 316 share ASTM A240 minimums: 515 MPa tensile, 205 MPa yield, 40 % elongation.
  • 304L and 316L limit carbon to 0.030 % to prevent weld sensitization.
  • A magnet cannot tell 304 from 316; use a molybdenum spot test, XRF or the mill certificate.

304 vs 316 stainless steel: the main difference

The main difference between 304 and 316 stainless steel is molybdenum. 316 contains 2–3 % molybdenum and more nickel, which gives it much better resistance to pitting and crevice corrosion in chlorides such as salt water. 304 has no specified molybdenum and costs less.

Both are austenitic chromium-nickel stainless steels. They look the same, weigh almost the same, have the same minimum strength in the annealed condition, are both non-magnetic when annealed, and weld and form in much the same way. In practice the choice comes down to one question: will the part see chlorides? If yes, 316. If no, 304 does the job for less money.

304 is about 18 % chromium and 8 % nickel, the classic 18-8 stainless. 316 trades a little chromium (16–18 %) for 10–14 % nickel and 2–3 % molybdenum. More on the families and naming is in stainless steel grades explained.

304 vs 316 comparison chart

This 304 vs 316 comparison chart puts composition, pitting resistance, minimum mechanical properties and designations side by side. Composition ranges and properties are the ASTM A240 limits for annealed plate, sheet and strip.

Property304316
FamilyAustenitic chromium-nickelAustenitic chromium-nickel-molybdenum
Nominal name18-8 (18Cr-8Ni)about 17Cr-12Ni-2Mo
Chromium, %18.0–20.016.0–18.0
Nickel, %8.0–10.510.0–14.0
Molybdenum, %none specified2.0–3.0
Carbon, max %0.07 (304L: 0.03)0.08 (316L: 0.03)
Typical PREN≈ 18–20≈ 24–26
Tensile strength, min515 MPa (75 ksi)515 MPa (75 ksi)
Yield strength (0.2 %), min205 MPa (30 ksi)205 MPa (30 ksi)
Elongation in 50 mm, min40 %40 %
Magnetic (annealed)No; slightly after cold workNo; stays less magnetic after cold work
Hardenable by heat treatmentNo, cold work onlyNo, cold work only
Density, typical≈ 7.9–8.0 g/cm³≈ 8.0 g/cm³
ISO 3506 fastener classA2A4
Relative costBaseTypically 20–40 % more
UNSS30400S31600
EN number1.43011.4401

Strength figures are specified minimums, not typical values; actual material usually exceeds them. Other product standards (A276 bar, A312 pipe, A479 bar) have their own limits. The cost premium for 316 is typical and moves with nickel and molybdenum surcharges. The governing standard and the mill certificate decide.

304 vs 316 corrosion resistance

316 has clearly better corrosion resistance than 304 in chlorides. Its typical PREN (Pitting Resistance Equivalent Number) is about 24–26, against about 18–20 for 304.

PREN = %Cr + 3.3 × %Mo + 16 × %N. Molybdenum counts 3.3 times as much as chromium, so 2 % Mo adds about 6.6 points, more than 316 gives up in chromium. The practical results:

  • Indoors, fresh water, inland air, most food: 304 and 316 both perform well. 304 is the economical choice.
  • Coastal air, road salt, pools, brines: 304 tends to tea-stain and pit; 316 holds up much better.
  • Chloride-containing chemicals and cleaners: 316 is the usual minimum.
  • Seawater immersion and warm chlorides: both are marginal or unsuitable; duplex 2205 or higher alloys are used.

316 does not fix every corrosion problem. Both grades are prone to chloride stress-corrosion cracking in warm chloride solutions, generally above about 60 °C (140 °F), and both can crevice-corrode under gaskets and deposits. See does stainless steel rust for causes and prevention.

Which is stronger, 304 or 316 stainless steel?

Neither is stronger by specification. Under ASTM A240, annealed 304 and 316 have the same minimums: 515 MPa (75 ksi) tensile strength, 205 MPa (30 ksi) yield strength and 40 % elongation.

Real heats of either grade often test above those minimums, and the spread between heats is usually larger than the difference between grades. 316 is generally credited with somewhat better strength at high temperature because of its molybdenum. Hardness in the annealed condition is similar, and A240 caps it for both. Neither grade hardens by heat treatment; both gain strength and hardness only by cold work, which is why cold-drawn bar and cold-headed fasteners are much stronger than annealed plate.

For strength-critical stainless parts, look at other grades: 2205 duplex has a minimum yield of 450 MPa (65 ksi) under A240, and precipitation-hardening 17-4PH is stronger still after ageing. For bolted joints in stainless, galling and lower clamp loads matter more than grade; see bolt preload and clamp load and the bolt torque chart.

304L and 316L: the low-carbon L grades

304L and 316L are the low-carbon versions of 304 and 316, with carbon limited to 0.030 % maximum. Low carbon prevents weld sensitization, so welded parts keep their corrosion resistance without a post-weld anneal.

When a standard-carbon austenitic grade spends time between about 425 and 815 °C (800 and 1500 °F), as the heat-affected zone of a weld does, chromium carbides form at the grain boundaries. The metal next to them loses chromium and can suffer intergranular corrosion. With 0.03 % carbon there is too little carbon to form damaging amounts of carbide in normal welding. The trade-off is a slightly lower specified minimum strength:

GradeCarbon, max %Tensile, minYield, minElongation, min
3040.07515 MPa (75 ksi)205 MPa (30 ksi)40 %
304L0.030485 MPa (70 ksi)170 MPa (25 ksi)40 %
3160.08515 MPa (75 ksi)205 MPa (30 ksi)40 %
316L0.030485 MPa (70 ksi)170 MPa (25 ksi)40 %

Values are ASTM A240 minimums for annealed material. Much plate, sheet and pipe is dual-certified 304/304L or 316/316L, meaning it meets the low carbon limit of the L grade and the strength of the straight grade. For heavy welded sections, tanks and pipework, specify 304L or 316L. In machined parts that are never welded, 304 and 304L behave practically the same.

304 and 316 equivalents: EN, JIS and GB

304 is nearest to EN 1.4301 and JIS SUS304; 316 is nearest to EN 1.4401 and JIS SUS316. The L grades map to 1.4307 and 1.4404. The table comes from the site's steel equivalents chart.

AISI / ASTMUNSEN numberEN nameJISChina GB
304S304001.4301X5CrNi18-10SUS30406Cr19Ni10
304LS304031.4307X2CrNi18-9SUS304L022Cr19Ni10
316S316001.4401X5CrNiMo17-12-2SUS31606Cr17Ni12Mo2
316LS316031.4404X2CrNiMo17-12-2SUS316L022Cr17Ni12Mo2

These are nearest equivalents, not identical grades. EN 1.4401 and ASTM 316 overlap but differ in detail, for example in nickel and molybdenum limits, so a drawing that calls for one does not automatically accept the other. EN 1.4404 is the usual European choice where an American drawing says 316L.

How to tell 304 from 316 stainless steel

You cannot tell 304 from 316 by eye, weight or magnet. The reliable ways are a molybdenum spot test, a handheld XRF analyzer or optical emission spectrometer, and the mill certificate traced to the heat number.

  • Magnet: useless here. Both are non-magnetic when annealed and both can become slightly magnetic after cold work.
  • Molybdenum spot test: a reagent kit, often applied with a small electric current, changes color when molybdenum is present. It separates 316 from 304 but does not confirm the exact grade.
  • XRF or OES analysis: handheld XRF reads chromium, nickel and molybdenum in seconds and is the standard tool for positive material identification. It cannot read carbon reliably, so it cannot separate 316 from 316L; OES can.
  • Markings and paperwork: pipe, plate and bar from reputable mills carry grade and heat markings that match a mill test certificate. Keep offcuts marked.
  • Fasteners: metric stainless bolts are head-marked A2 (304-type) or A4 (316-type) under ISO 3506. An inch bolt marked 18-8 is a 300 series grade without molybdenum, not 316.

Which is better, 304 or 316? Food grade and marine grade

316 is better for salt, chlorides and marine use; 304 is better value everywhere else. Both are standard food-contact stainless steels; 316 is chosen where foods or cleaning chemicals are salty or acidic.

Food grade. "Food grade" is not a grade name. 304 is the default for food, dairy, brewing and catering equipment, sinks and benches. 316 is used for brines, sauces, pickling, salty and acidic products, and equipment cleaned with aggressive chloride-containing chemicals. Food-contact compliance also depends on finish, design and the applicable regulations, not on grade alone.

Marine grade. "Marine grade" usually means 316 or 316L. Use it for boat hardware, seafront railings, coastal architecture and anything within reach of salt spray, together with A4 fasteners and a smooth finish. Do not mix a 304 fastener into 316 hardware; the 304 part corrodes first.

Machining. 316 is slightly gummier and tougher to machine than 304; both work-harden. Free-machining 303 is the easy-machining alternative for parts that are not welded or exposed to chlorides. See 303 vs 304 stainless steel for a 303 vs 304 vs 316 machining comparison, and drill bits for metal for drilling stainless.

Sources and standards

  • EN 10088-1, Stainless steels, list of stainless steels
  • ASTM A240
  • ASTM A276
  • ISO 3506-1

General reference information. When a manufacturer, drawing or governing standard gives a value, that value takes precedence.

Related charts and guides

Common questions

What is the difference between 304 and 316 stainless steel?

316 contains 2–3 % molybdenum and 10–14 % nickel, while 304 has about 18–20 % chromium, 8–10.5 % nickel and no specified molybdenum. The molybdenum gives 316 much better resistance to pitting and crevice corrosion in salt and chlorides. Strength, appearance, magnetism and weldability are practically the same, and 316 typically costs 20–40 % more.

Which is better, 304 or 316 stainless steel?

316 is better wherever salt or chlorides are present: marine hardware, coastal buildings, pools, brines and chloride chemicals. In indoor, fresh-water and inland use, 304 performs just as well and costs less, so it is the better choice there. For warm seawater or immersion, neither is ideal and duplex 2205 is often used.

Which is stronger, 304 or 316 stainless steel?

Neither is stronger by specification. ASTM A240 gives annealed 304 and 316 the same minimums: 515 MPa (75 ksi) tensile strength, 205 MPa (30 ksi) yield strength and 40 % elongation. Real heats vary more than the grades differ. Both gain strength only by cold work, not heat treatment.

Is 316 stainless steel magnetic?

Annealed 316 is non-magnetic, like annealed 304. Its higher nickel content makes it less likely than 304 to become magnetic after cold working, but heavily formed areas and welds can still attract a magnet slightly. A magnet test therefore cannot reliably tell 304 from 316; use a molybdenum spot test or XRF.

What is the difference between 304 and 304L?

304L limits carbon to 0.030 % maximum, against 0.07 % for 304 under ASTM A240. The low carbon prevents chromium carbide formation, called sensitization, in the heat-affected zone of welds, so welded parts keep their corrosion resistance. 304L has slightly lower minimums: 485 MPa (70 ksi) tensile and 170 MPa (25 ksi) yield. Much material is dual-certified 304/304L.

How can you tell 304 from 316 stainless steel?

Use a molybdenum spot-test kit, a handheld XRF analyzer or an optical emission spectrometer, or check the mill certificate against the heat number marked on the material. 316 contains 2–3 % molybdenum and 304 does not. A magnet, a file, appearance and weight cannot separate the two grades.

Is 316 stainless steel food grade?

Yes, 316 is widely used for food-contact equipment, as is 304. 304 is the default for dairy, brewing and catering equipment; 316 is chosen for salty, acidic or brined foods and for equipment cleaned with aggressive chloride-containing chemicals. Food-contact compliance also depends on surface finish, hygienic design and the applicable regulations.

What is the European equivalent of 316 stainless steel?

The nearest European equivalent of 316 is EN 1.4401, steel name X5CrNiMo17-12-2. For 316L it is EN 1.4404, X2CrNiMo17-12-2. These are nearest equivalents, not identical grades, because composition limits differ in detail. The governing standard and the mill certificate decide whether a material meets a drawing.